Nanoindentation

  • 18 min read
  • 5 chapters

Related on Lably

Through List of materials properties, Hardness and Micrometre

Background

In a traditional indentation test (macro or micro indentation), a hard tip whose mechanical properties are known (frequently made of a very hard material like diamond) is pressed into a sample whose properties are unknown. The load placed on the indenter tip is increased as the tip penetrates further into the specimen and soon reaches a user-defined value. At this point, the load may be held constant for a period or removed. The area of the residual indentation in the sample is measured and the hardness, H, is defined as the maximum load, Pmax, divided by the residual indentation area, Ar:

H=PmaxAr.

For most techniques, the projected area may be measured directly using light microscopy. As can be seen from this equation, a given load will make a smaller indent in a "hard" material than a "soft" one.

This technique is limited due to large and varied tip shapes, with indenter rigs which do not have very good spatial resolution (the location of the area to be indented is very hard to specify accurately). Comparison across experiments, typically done in different laboratories, is difficult and often meaningless. Nanoindentation improves on these macro- and micro-indentation tests by indenting on the nanoscale with a very precise tip shape, high spatial resolutions to place the indents, and by providing real-time load-displacement (into the surface) data while the indentation is in progress.

In nanoindentation small loads and tip sizes are used, so the indentation area may only be a few square micrometres or even nanometres. This presents problems in determining the hardness, as the contact area is not easily found. Atomic force microscopy or scanning electron microscopy techniques may be utilized to image the indentation, but can be quite cumbersome. Instead, an indenter with a geometry known to high precision (usually a Berkovich tip, which has a three-sided pyramid geometry) is employed. During the course of the instrumented indentation process, a record of the depth of penetration is made, and then the area of the indent is determined using the known geometry of the indentation tip. While indenting, various parameters such as load and depth of penetration can be measured. A record of these values can be plotted on a graph to create a load-displacement curve (such as the one shown in Figure 1). These curves can be used to extract mechanical properties of the material.

Young's modulus

The slope of the curve, dP/dh, upon unloading is indicative of the stiffness S of the contact. This value generally includes a contribution from both the material being tested and the response of the test device itself. The stiffness of the contact can be used to calculate the reduced Young's modulus Er:

Er=1βπ2SAp(hc),

where Ap(hc) is the projected area of the indentation at the contact depth hc, and β is a geometrical constant on the order of unity. Ap(hc) is often approximated by a fitting polynomial as shown below for a Berkovich tip:

Ap(hc)=C0hc2+C1hc1+C2hc1/2+C3hc1/4+…+C8hc1/128

where C0 for a Berkovich tip is 24.5 while for a cube corner (90°) tip is 2.598. The reduced modulus Er is related to Young's modulus Es of the test specimen through the following relationship from contact mechanics:

1/Er=(1−νi2)/Ei+(1−νs2)/Es.

Here, the subscript i indicates a property of the indenter material and ν is Poisson's ratio. For a diamond indenter tip, Ei is 1140 GPa and νi is 0.07. Poisson's ratio of the specimen, νs, generally varies between 0 and 0.5 for most materials (though it can be negative) and is typically around 0.3.

There are two different types of hardness that can be obtained from a nano indenter: one is as in traditional macroindentation tests where one attains a single hardness value per experiment; the other is based on the hardness as the material is being indented resulting in hardness as a function of depth.

H=PmaxAr.

Hardness

The hardness is given by the equation above, relating the maximum load to the indentation area. The area can be measured after the indentation by in-situ atomic force microscopy, or by 'after-the event' optical (or electron) microscopy. An example indentation image, from which the area may be determined, is shown at right.

Some nanoindenters use an area function based on the geometry of the tip, compensating for elastic load during the test. Use of this area function provides a method of gaining real-time nanohardness values from a load-displacement graph. However, there is some controversy over the use of area functions to estimate the residual areas versus direct measurement. An area function Ap(hc) typically describes the projected area of an indent as a 2nd-order polynomial function of the indenter depth h. When too many coefficients are used, the function will begin to fit to the noise in the data, and inflection points will develop. If the curve can fit well with only two coefficients, this is the best. However, if many data points are used, sometimes all 6 coefficients will need to be used to get a good area function. Typically, 3 or 4 coefficients works well. Service Document Probe Calibration; CSV-T-003 v3.0; Exclusive application of an area function in the absence of adequate knowledge of material response can lead to misinterpretation of resulting data. Cross-checking of areas microscopically is to be encouraged.

Strain-rate sensitivity

The strain-rate sensitivity of the flow stress m is defined as

m=∂ln⁡σ∂ln⁡ε˙,

where σ=σ(ε˙) is the flow stress and ε˙ is the strain rate produced under the indenter. For nanoindentation experiments which include a holding period at constant load (i.e. the flat, top area of the load-displacement curve), m can be determined from

dln⁡H=mdln⁡εp˙+ndln⁡hp.

The subscripts p indicate these values are to be determined from the plastic components only.

Activation volume

Interpreted loosely as the volume swept out by dislocations during thermal activation, the activation volume V∗ is

V∗=9kBT∂ln⁡ε˙∂H,

where T is the temperature and kB is the Boltzmann constant. From the definition of m, it is easy to see that V∗∝(Hm)−1.